Mo2TiC2Tx preparation method

source:beike new material Views:5763time:2020-08-10 QQ Academic Group: 1092348845

Preparation method of Mo2TiC2Tx: Slowly add 2g of Mo2TiAlC2 to 20ml of 50% HF solution, and keep stirring at 55 degrees Celsius for 72 hours. Subsequently, the sample was washed with deionized water multiple times by centrifugation until the pH value was close to about 6, and the resulting precipitate was a multilayer Mo2TiC2Tx. Next, take 2g of the dried multilayer Mo2TiC2Tx and re-disperse it in 50ml of deionized water, and add 1ml of 40% mass fraction of tetrabutylammonium hydroxide (TBAOH), continue stirring for 1 hour, and then sonicate for 1 hour under Ar atmosphere . Finally, centrifuge at 3500 rpm for 1 hour, and the resulting upper suspension is the stripped Mo2TiC2Tx solution (delaminated Mo2TiC2Tx, d-Mo2TiC2Tx).


 

Reminder: Beijing Beike New Material Technology Co., Ltd. supplies products only for scientific research, not for humans
All rights reserved © 2019 beijing beike new material Technology Co., Ltd 京ICP备16054715-2号
advisory
phone
Email:mxenes@163.com
Tel:+86-17715390137
scan

scan
WeChat